Influence of Thickness on TNDT of Drop-weight Specimen
-
Graphical Abstract
-
Abstract
Based on the data of Drop-weight test of various kinds of specimens with different thickness, it could be concluded that the value of TNDT is not only dependent on the materials but also the thickness of the specimen. The relationship between TNDT and thickness could be described by a function of: TNDT=At-m+B, where A、B、m are coefficients related with the materials. Therefore, the six type of specimens (P1~P6) with thickness 12~50mm and their test conditions are recommended in engineering design in which the failure characteristic of materials should be properly described for the reliability of the design.
-
-